Zirconia specs and sintering programs
The published figures for the three series we stock, side by side. Every disc is 98 mm across and 10 mm to 25 mm thick, manufactured to ISO 13356. Materials are FDA-listed.
Where the series differ
Strength and translucency as published by the manufacturer.
3D PRO
- Flexural strength
- 650–1100 MPa
- Translucency
- 42–49%
- Sintering temperature
- 1500 °C
- Y2O3
- 4.5–10%
- Al2O3
- < 0.15%
Anterior through posterior, in one disc
ST Multilayer
- Flexural strength
- 1100 MPa
- Translucency
- 43%
- Sintering temperature
- 1530 °C
- Y2O3
- 4.5–6.0%
- Al2O3
- < 0.15%
Crowns and bridges, full-contour posteriors
HT White
- Flexural strength
- 1350 MPa
- Translucency
- 37%
- Sintering temperature
- 1530 °C
- Y2O3
- 4.5–6.0%
- Al2O3
- < 0.25%
Copings, frameworks, bridges, full arch
What all three share
- Density after sintering
- ≥ 6.0 g/cm³
- CTE (25–500 °C)
- (10 ± 0.5) × 10−6 K−1
- Monoclinic phase after accelerated aging
- < 15%
- Chemical solubility after sintering
- < 100 µg/cm²
- Radioactivity
- < 0.1 Bq/g
- ZrO2 + HfO2 + Y2O3
- > 99%
- Other oxides
- < 0.5%
Sintering programs
The manufacturer's published curves. The ramps and holds are the same for every series; only the final temperature changes. Times are holds, not totals.
| Rate | To | Then |
|---|---|---|
| 10 °C/min | 900 °C | Hold 30 min |
| 3 °C/min | 1300 °C | Hold 10 min |
| 3 °C/min | 1500 °C or 1530 °C | Hold 120 min |
| 8 °C/min | 300 °C | Cool naturally |
Verify your furnace's calibration before the first production run, and do not open the chamber above 300 °C. If you run a high-speed program, or the case is longer than three units, send it to us and we will confirm the schedule rather than have you infer one.
Units coming out wrong? Work through the sintering checklist.
Questions about the numbers
- What temperature do I sinter these zirconia discs at?
- 3D PRO at 1500 °C. ST Multilayer and HT White at 1530 °C. All three hold for 120 minutes at that temperature.
- How long does the sintering program take?
- About 10 hours from room temperature down to 300 °C, worked out from the published ramps and holds, then natural cooling.
- Can I use a high-speed program?
- We publish the conventional program only. If you run a high-speed program, or the case is longer than three units, email lab@hizir3d.com and we will confirm the schedule.
- Do you supply other zirconia grades?
- Yes, UT (highest esthetics) and ST PLUS (balanced esthetics and strength) in White, Preshaded and Multilayer, and ST in White and Preshaded, on request. They are not sold online, so email lab@hizir3d.com for specifications, shades and price.
Other grades on request. We also supply UT (highest esthetics) and ST PLUS (balanced esthetics and strength) in White, Preshaded and Multilayer, and ST in White and Preshaded. They are not sold online, so email lab@hizir3d.com for specifications, shades and price.